Janka hardness scale
The Janka test presses a 0.444-inch (11.28 mm) steel ball into a wood sample to half the ball's diameter; the side-hardness load required, in pounds-force, is the rating. Values here are at 12% moisture content per ASTM D143, from the USDA Wood Handbook, Table 5-3b. Click a column header to re-sort.
| Rank | Species | Janka lbf | Newtons | SG (green) | Type |
|---|---|---|---|---|---|
| 1 | Shagbark Hickory | 1,880 | 8,363 | 0.64 | hardwood |
| 2 | Black Locust | 1,700 | 7,562 | 0.66 | hardwood |
| 3 | Sugar Maple | 1,450 | 6,450 | 0.56 | hardwood |
| 4 | White Oak | 1,360 | 6,050 | 0.6 | hardwood |
| 5 | White Ash | 1,320 | 5,872 | 0.55 | hardwood |
| 6 | American Beech | 1,300 | 5,783 | 0.56 | hardwood |
| 7 | Red Oak | 1,290 | 5,738 | 0.56 | hardwood |
| 8 | Yellow Birch | 1,260 | 5,605 | 0.55 | hardwood |
| 9 | Black Walnut | 1,010 | 4,493 | 0.51 | hardwood |
| 10 | Black Cherry | 950 | 4,226 | 0.47 | hardwood |
| 11 | Red Maple | 950 | 4,226 | 0.49 | hardwood |
| 12 | Longleaf Pine | 870 | 3,870 | 0.54 | softwood |
| 13 | Sweetgum | 850 | 3,781 | 0.46 | hardwood |
| 14 | American Elm | 830 | 3,692 | 0.46 | hardwood |
| 15 | Western Larch | 830 | 3,692 | 0.48 | softwood |
| 16 | Douglas Fir | 710 | 3,158 | 0.45 | softwood |
| 17 | Shortleaf Pine | 690 | 3,069 | 0.47 | softwood |
| 18 | Southern Yellow Pine (Loblolly) | 690 | 3,069 | 0.47 | softwood |
| 19 | Interior Douglas Fir | 660 | 2,936 | 0.46 | softwood |
| 20 | Red Alder | 590 | 2,624 | 0.37 | hardwood |
| 21 | Tamarack | 590 | 2,624 | 0.49 | softwood |
| 22 | Alaska Yellow Cedar | 580 | 2,580 | 0.42 | softwood |
| 23 | Red Pine | 560 | 2,491 | 0.41 | softwood |
| 24 | Hem-Fir (Western Hemlock) | 540 | 2,402 | 0.42 | softwood |
| 25 | Yellow Poplar | 540 | 2,402 | 0.4 | hardwood |
| 26 | Red Spruce | 530 | 2,358 | 0.37 | softwood |
| 27 | Baldcypress | 510 | 2,269 | 0.42 | softwood |
| 28 | Sitka Spruce | 510 | 2,269 | 0.37 | softwood |
| 29 | Eastern Hemlock | 500 | 2,224 | 0.38 | softwood |
| 30 | Grand Fir | 490 | 2,180 | 0.35 | softwood |
| 31 | Lodgepole Pine | 480 | 2,135 | 0.38 | softwood |
| 32 | Redwood | 480 | 2,135 | 0.38 | softwood |
| 33 | White Fir | 480 | 2,135 | 0.37 | softwood |
| 34 | Incense Cedar | 470 | 2,091 | 0.35 | softwood |
| 35 | Ponderosa Pine | 460 | 2,046 | 0.38 | softwood |
| 36 | Eastern Cottonwood | 430 | 1,913 | 0.37 | hardwood |
| 37 | Western White Pine | 420 | 1,868 | 0.35 | softwood |
| 38 | Basswood | 410 | 1,824 | 0.32 | hardwood |
| 39 | SPF (White Spruce) | 410 | 1,824 | 0.33 | softwood |
| 40 | Engelmann Spruce | 390 | 1,735 | 0.33 | softwood |
| 41 | Balsam Fir | 380 | 1,690 | 0.33 | softwood |
| 42 | Eastern White Pine | 380 | 1,690 | 0.34 | softwood |
| 43 | Sugar Pine | 380 | 1,690 | 0.34 | softwood |
| 44 | Quaking Aspen | 350 | 1,557 | 0.35 | hardwood |
| 45 | Western Red Cedar | 350 | 1,557 | 0.31 | softwood |
| 46 | Northern White Cedar | 320 | 1,423 | 0.29 | softwood |
Hardness measures resistance to denting, not how much a board weighs — the two correlate loosely, not exactly. Red Alder is a good example: it ranks #20 for hardness but #31 for density among these 46 species. For density alone, see the wood density chart; individual profiles: Hickory, Red Alder.